Entanglement Molecular Weights
Polymer/ Entanglement Weight | Me1 (g/mol) |
Poly(octadecyl methacrylate) | 225140 |
Poly(dodecyl methacrylate) | 112050 |
Poly(tetradecyl methacrylate) | 92440 |
Poly(4-tert-butylphenyl methacrylate) | 64850 |
Poly(decyl methacrylate) | 61120 |
Poly(2-chlorophenyl methacrylate) | 52040 |
Poly(4-tert-butylcyclohexyl methacrylate) | 50020 |
Poly(phenyl methacrylate) | 45440 |
Poly(cyclohexylethene) | 44120 |
Poly(cyclohexyl methacrylate), PCHMA | 34690 |
Poly(hexyl methacrylate) | 33450 |
Poly(tert-butyl methacrylate) | 28260 |
Poly(4-tert-butylstyrene) | 21675 |
Polystyrene, PS | 16910 |
Poly(α-methylstyrene) | 16370 |
Poly(1-butene), PB-1 | 12260 |
Poly(methyl methacrylate), PMMA | 11325 |
Poly(methyl acrylate), PMA | 10035 |
Poly(vinyl acetate) | 9680 |
Poly(ethyl acrylate), PEA | 8180 |
Poly(isobutene) | 7935 |
Poly(isopentene) | 6580 |
Poly(vinyl chloride), PVC | 5410 |
Poly(tetrafluoroethene), PTFE | 4650 |
Poly(propylene) | 4595 |
Poly(1-methyl-1-butenylene) | 4085 |
Poly(tetramethyl bisphenol A isophthalate) | 3970 |
PoIy(1,2-butadiene) | 3710 |
Poly(2,6-dimethyl-p-phenylene oxide), PPO | 3570 |
Poly(tetramethyl Bisphenol A carbonate) | 3420 |
Polyacetal, Poly(methylene oxide), POM | 2560 |
Poly(Bisphenol A carbonate), PC | 2510 |
Poly(caprolactam), Nylon 6 | 2490 |
Poly(1,3-butadiene) | 2480 |
Poly(bisphenol A isophthalate) | 2450 |
Poly(1,4-butadiene) | 2380 |
Polysulfone, PSU | 2315 |
Poly(hexamethylene adipamide), Nylon 6,6 | 2010 |
Poly(hexane-1,6-diyl isophthalamide) | 1940 |
Poly(ethylene glycol), PEG | 1850 |
Poly(Bisphenol-A diglycidyl ether), PDGEBA | 1570 |
Poly(ethylene terephthalate), PET | 1450 |
Poly(Bisphenol A terephthalate) | 1395 |
Poly(ethylene), PE | 1160 |